Title: help with D2 steel
Post by: Sharppoint on July 15, 2011, 10:38:00 AM
being fairly new to knife making whats the correct way to handle d2. not to oil quench or to air quench, some what confused.any help very thankfull.
Title: Re: help with D2 steel
Post by: kbaknife on July 15, 2011, 12:08:00 PM
D2
http://www.crucible.com/eselector/general/generalpart2.html    

Austenize @ 1825/l875
   
Hold 15-45 minutes
   
AIR quench
   
temper 400-1000
   
Rc hardness 62/55